24 grades · 24 cast
Leaded Bearing Bronze
High-lead tin bronzes (SAE 660, 80-10-10) for bearings and bushings. 24 grades across USA, European, German, British, Japanese and Chinese standards — each with its own datasheet and cross-reference.
24 of 24 grades
| Grade | Name | System | Form | Composition |
|---|---|---|---|---|
| C93200● data | Bearing bronze 83-7-7-3 (SAE 660) | USA · UNS | Cast | Cu 83, Sn 7, Pb 7, Zn 3 |
| C93500● data | High-leaded tin bronze 85-5-9-1 | USA · UNS | Cast | Cu 85, Sn 5, Pb 9, Zn 1 |
| C93700● data | Bearing bronze 80-10-10 (SAE 64) | USA · UNS | Cast | Cu 80, Sn 10, Pb 10 |
| C93800● data | High-leaded tin bronze 78-7-15 (SAE 67) | USA · UNS | Cast | Cu 78, Sn 7, Pb 15 |
| C94100● data | High-leaded tin bronze 70-5.5-20 | USA · UNS | Cast | Cu ~72, Sn ~5.5, Pb ~20, Zn ~2 |
| CC494K● data | CuSn5Pb9-C | Europe · EN 1982:2017 | Cast | Sn 4–6, Pb 8–10, Zn ≤ 2, Cu rem |
| CC495K● data | CuSn10Pb10-C | Europe · EN 1982:2017 | Cast | Sn 9–11, Pb 8–11, Cu rem |
| CC496K● data | CuSn7Pb15-C | Europe · EN 1982:2017 | Cast | Sn 6–8, Pb 13–17, Cu rem |
| CC497K● data | CuSn5Pb20-C | Europe · EN 1982:2017 | Cast | Sn 4–6, Pb 18–23, Cu rem |
| 2.1176● data | G-CuPb10Sn | Germany · DIN 1716 | Cast | Pb 8–11, Sn 9–11, Cu rem |
| 2.1182● data | G-CuPb15Sn | Germany · DIN 1716 | Cast | Pb 13–17, Sn 7–9, Cu rem |
| 2.1188● data | G-CuPb20Sn | Germany · DIN 1716 | Cast | Pb 18–23, Sn 4–6, Cu rem |
| LB1● data | LB1 | UK · BS 1400:1985 | Cast | Sn 8–10, Pb 13–17, Cu rem |
| LB2● data | LB2 | UK · BS 1400:1985 | Cast | Sn 9–11, Pb 8.5–11, Cu rem |
| LB4● data | LB4 | UK · BS 1400:1985 | Cast | Sn 4–6, Pb 8–10, Zn ≤ 2, Cu rem |
| LB5● data | LB5 | UK · BS 1400:1985 | Cast | Sn 4–6, Pb 18–23, Cu rem |
| CAC602● data | LBC2 | Japan · JIS H 5120 | Cast | Cu 82–86, Sn 9–11, Pb 4–6 |
| CAC603● data | LBC3 | Japan · JIS H 5120 | Cast | Cu 77–81, Sn 9–11, Pb 9–11 |
| CAC604● data | LBC4 | Japan · JIS H 5120 | Cast | Cu 74–78, Sn 7–9, Pb 14–16 |
| CAC605● data | LBC5 | Japan · JIS H 5120 | Cast | Cu 70–76, Sn 6–8, Pb 16–22 |
| ZCuPb10Sn10● data | ZCuPb10Sn10 | China · GB/T 1176-2013 | Cast | Pb 8–11, Sn 9–11, Cu rem |
| ZCuPb15Sn8● data | ZCuPb15Sn8 | China · GB/T 1176-2013 | Cast | Pb 13–17, Sn 7–9, Cu rem |
| ZCuPb20Sn5● data | ZCuPb20Sn5 | China · GB/T 1176-2013 | Cast | Pb 18–23, Sn 4–6, Cu rem |
| ZCuPb9Sn5● data | ZCuPb9Sn5 | China · GB/T 1176-2013 | Cast | Pb 8–10, Sn 4–6, Cu rem |
Overview
Leaded bearing bronzes are cast copper-tin alloys containing about 7–20% lead, designed for plain bearings, bushings, thrust washers and wear plates that must run against steel shafts with good conformability, embeddability and tolerance to imperfect lubrication. The workhorse grade is C93200 (SAE 660, 83-7-7-3), the most widely used bearing bronze in North America; the high-lead grades C93500, C93700 (SAE 64, 80-10-10), C93800 (SAE 67) and C94100 cover heavier loads, higher speeds or marginal lubrication. In Europe the equivalent family is CC494K–CC497K in EN 1982, and in Britain LB1, LB2, LB4 and LB5.
This guide explains how lead and tin work together in a bearing, how the grades differ, how they are cast (mostly continuous and centrifugal), and how to choose and specify a bronze bushing that lasts.
What a bearing alloy has to do
A plain bearing runs on a thin film of lubricant, but at start-up, under shock load or when lubrication is poor, the shaft touches the bearing surface. A good bearing alloy must therefore:
- Carry load without deforming (strength and hardness).
- Conform to slight misalignment and shaft deflection (softness and ductility).
- Embed small dirt particles so they do not score the shaft.
- Resist seizure when the oil film breaks down (compatibility with steel).
- Conduct heat away from the rubbing surface.
- Resist fatigue and corrosion in the lubricant and environment.
No single element gives all of these. Leaded tin bronzes balance them: tin supplies strength, lead supplies anti-seizure and embeddability, and the copper matrix supplies thermal conductivity and corrosion resistance.
The metallurgy in plain words
- Tin (about 5–10%) strengthens the copper and gives fatigue and load capacity. Higher tin means a harder, stronger bearing.
- Lead (about 7–20%) is insoluble in copper and appears as fine, evenly distributed pools. Under boundary lubrication the lead smears over the surface and acts as a solid lubricant, preventing seizure. It also makes the bearing more conformable and better at embedding dirt. More lead means better anti-seizure and conformability, but lower strength.
- Zinc (up to about 3%) deoxidizes the melt and slightly strengthens the alloy.
- Nickel (small amounts) helps keep lead evenly distributed and improves strength.
Because lead does not dissolve and is much heavier than copper, high-lead bronzes tend to segregate if cooled slowly. Continuous casting and centrifugal casting, which freeze the metal quickly, give the fine, uniform lead distribution a bearing needs.
The grades compared
| Grade (USA) | SAE | EN / BS / JIS / GB | Nominal Cu-Sn-Pb-Zn | Character | Typical uses |
|---|---|---|---|---|---|
| C93200 | 660 | — (closest EN: CC493K–CC494K range) | 83-7-7-3 | General-purpose; best all-round balance | Bushings, bearings, thrust washers in machinery |
| C93500 | — | CC494K / LB4 / CAC602 / ZCuPb9Sn5 | 85-5-9-1 | Good conformability, moderate loads | Bushings, plain bearings, wear plates |
| C93700 | 64 | CC495K / 2.1176 / LB2 / CAC603 / ZCuPb10Sn10 | 80-10-10 | High strength + good anti-seizure; heavy loads and higher speeds | Heavy-duty and high-speed bearings, rolling-mill bearings |
| C93800 | 67 | CC496K / 2.1182 / LB1 / CAC604 / ZCuPb15Sn8 | 78-7-15 | Very good under marginal lubrication | Bearings with poor lubrication or dirt |
| C94100 | — | CC497K / 2.1188 / LB5 / CAC605 / ZCuPb20Sn5 | 70-5.5-20-2 | Highest lead; best conformability, lowest strength | Light-load bearings, wear plates, thrust washers |
Typical properties
Typical ranges based on ASTM B505 (continuous castings), B271 (centrifugal) and B584 (sand) and EN 1982 data. Continuous and centrifugal castings are usually stronger than sand castings. The governing standard and the material test certificate define actual values.
| Property | C93200 (SAE 660) | C93700 (SAE 64) | C93800 (SAE 67) | C94100 |
|---|---|---|---|---|
| Tensile strength | Typically about 200–260 MPa | Typically about 200–270 MPa | Typically about 170–220 MPa | Typically about 150–200 MPa |
| 0.2% proof strength | About 100–140 MPa | About 85–130 MPa | About 85–110 MPa | About 70–100 MPa |
| Elongation | About 10–20% | About 10–20% | About 5–15% | About 5–15% |
| Hardness | About 60–70 HB | About 60–75 HB | About 50–60 HB | About 45–55 HB |
| Machinability (C36000 = 100) | About 70 | About 80 | About 80 | About 80 |
Casting methods that suit bearing bronzes
- Continuous casting — the standard source of bushing stock: solid and hollow bars in many diameters, with fine, uniform structure. Bushings are then machined in volume.
- Centrifugal casting — for larger bushings, sleeves and rings; produces dense, uniform walls.
- Sand casting — for flanged bearings, split bearing halves, slide plates, housings with integral bearing surfaces and large, non-cylindrical parts.
- Shell or gravity die casting — for smaller shaped bearing parts in volume.
Conex produces bronze bushings and bearings by centrifugal, continuous and sand casting and finishes them on CNC lathes, including oil grooves, flanges and split halves.
Applications by industry
| Industry | Parts | Usual grades |
|---|---|---|
| General engineering & machine tools | Bushings, guides, slideways, thrust washers | C93200 |
| Steel, cement, sugar & heavy machinery | Rolling-mill bearings, crusher bushes, heavy roll bearings | C93700, C93200 |
| Earthmoving & agriculture | Pivot bushes, pin bushes in dirty conditions | C93800, C93700 |
| Pumps & compressors | Line-shaft bearings, wear rings | C93200, C93500 |
| Railways | Suspension and linkage bushes, wear plates | C93200, C93700 |
| Material handling | Wheel and roller bushes, sheave bushes | C93200 |
How to choose between grades
- Normal load, good lubrication, general machinery? C93200 (SAE 660).
- Heavy load, possibly high speed, or shock? C93700 (SAE 64 / LB2 / CC495K).
- Marginal lubrication, dirt or misalignment? C93800 (SAE 67 / LB1) or C94100 for light loads.
- Very heavy, slow loads? Consider tin bronze, aluminum bronze or high-tensile brass instead of a leaded bronze.
- Corrosive water or seawater? Consider tin bronze or aluminum bronze; high-lead bronzes are less suited to corrosive service.
Design tips for bronze bushings
- Shaft hardness and finish: a hardened, ground steel shaft with a fine finish greatly extends bushing life.
- Clearance: allow running clearance appropriate to diameter, speed and temperature; too little causes seizure, too much causes knocking.
- Length-to-diameter ratio: roughly 1 to 1.5 is common; very long bushes are sensitive to misalignment.
- Interference fit: bushes are usually press-fitted; allow for bore close-in after pressing and finish-machine the bore after fitting if accuracy is critical.
- Lubrication grooves: place them in the unloaded zone and round their edges.
- Wall thickness: thick enough to resist distortion during press-fitting.
Equivalents across standards
| USA | EN 1982 | DIN | BS 1400 (withdrawn) | JIS | GB |
|---|---|---|---|---|---|
| C93700 | CC495K CuSn10Pb10-C | 2.1176 | LB2 | CAC603 | ZCuPb10Sn10 |
| C93800 | CC496K CuSn7Pb15-C | 2.1182 | LB1 | CAC604 | ZCuPb15Sn8 |
| C94100 | CC497K CuSn5Pb20-C | 2.1188 | LB5 | CAC605 | ZCuPb20Sn5 |
| C93500 | CC494K CuSn5Pb9-C | — | LB4 | CAC602 | ZCuPb9Sn5 |
C93200 (SAE 660) has no exact EN equivalent; CC493K (CuSn7Zn4Pb7-C, Rg7) is often used in its place in Europe. Equivalents are approximate — quote the governing standard.
Common mistakes
- Using a soft high-lead bronze for heavy, slow loads — it will deform. Use C93700, tin bronze or aluminum bronze.
- Running a bronze bushing on a soft, rough shaft.
- Machining the bore before press-fitting on tight-tolerance assemblies, then finding it undersize.
- Sand casting simple bushings that would be cheaper and better from continuous or centrifugal stock.
- Using leaded bronze in potable-water equipment where lead is restricted.
Quality checks and documents
Every melt is analyzed by spectrometer, with lead and tin checked against the grade. Bushings are inspected for dimensions, bore finish and concentricity; hardness is checked; test bars or samples are tensile tested where specified; and the structure can be examined for lead distribution on request. Material test certificates (EN 10204 3.1 on request) are supplied under an ISO 9001:2015 quality system.
How a leaded bronze bearing actually works
Under a microscope, a leaded tin bronze looks like a strong copper-tin matrix with small pockets of lead scattered through it. Lead does not dissolve in copper, so it stays as separate soft particles. In service, those particles do three useful things. They smear across the surface if the oil film breaks down, acting as an emergency lubricant and preventing seizure. They let hard dirt particles bed into the surface instead of scoring the shaft, which is called embeddability. And they help the bearing conform to small misalignments. The copper-tin matrix carries the load. The more lead, the more forgiving the bearing becomes, but the lower its strength and fatigue resistance.
Choosing lead content by duty
- Around 7 percent lead (C93200 / SAE 660): the general-purpose bearing bronze for moderate loads and speeds, with a good balance of strength and anti-seizure behavior.
- Around 10 percent lead (C93700, CuSn10Pb10 / CC495K): higher loads with marginal lubrication, good for hydraulic pump parts and heavily loaded bushes.
- Around 15 to 25 percent lead (C93800, C94300, CuSn7Pb15 / CC496K): poor lubrication, dirty conditions, misalignment and low loads, such as conveyor and agricultural bearings.
Running-in and lubrication
New bronze bearings benefit from a gentle running-in period at reduced load, which smooths the surface and builds a stable oil film. Oil grooves should carry lubricant to the unloaded side of the bearing and spread it into the loaded zone without cutting across it. Grease-lubricated bushes need regular greasing; where that is impractical, graphite-plugged bronze or a higher-lead grade is a better choice.
Lead and the environment
Leaded bronzes remain widely used and accepted for industrial bearings, but they are not suitable for drinking-water or food-contact parts, and some markets restrict lead in certain products. Lead-free bearing alternatives using bismuth or other elements exist; buyers who need them should state the requirement and the applicable regulation.
Specifying leaded bearing bronze on a drawing
Examples: "Continuous-cast bronze C93200 to ASTM B505", "Centrifugally cast CuSn10Pb10 (CC495K) to EN 1982", "Leaded tin bronze LB2 (legacy BS 1400)". Add hardness if required, the shaft hardness and finish, oil grooves, and the inspection and certificate requirements.
Working with Conex on bearing bronzes
Conex casts leaded tin bronzes by continuous, centrifugal and sand casting in Jamnagar, machines bushes, bearings and thrust washers in-house on CNC equipment, and supplies them with chemical analysis, hardness results and material test certificates under an ISO 9001:2015 quality system to customers in more than 34 countries.
Common bearing shapes
Leaded bronze is supplied as plain cylindrical bushes, flanged bushes, thrust washers, split bearing shells, slide plates and wear strips, as well as solid and hollow bar for in-house machining. Continuous-cast bar is the quickest route for small and medium bushes in many sizes.
Ordering tips
Give the shaft diameter and tolerance, the housing bore, the bush length, the type of lubrication and the operating load and speed. With that information the alloy, fit and groove pattern can be confirmed before machining starts.
Bearing spares
Keep a few spare bushes for each critical machine; continuous-cast stock makes repeat orders quick.
Before you send an enquiry
A short list of facts helps choose the right grade from this family and quote accurately the first time:
- The part and its job: what it does, what it touches, and what a failure would cost in downtime or safety.
- Service conditions: fluid or environment, temperature range, pressure, loads, speed and lubrication.
- Grade or standard on the drawing: the UNS, EN, BS, JIS, GB, DIN or IS designation, or the old grade name if that is all you have.
- Process or stock form: sand, centrifugal, continuous, gravity die or investment casting, or bar and plate. The most economical route can be suggested for your quantity.
- Machining stage: rough cast, semi-finished with allowance, or fully finished to drawing.
- Tests and documents: chemical analysis, mechanical and hardness tests, pressure test, NDT, material test certificate type (EN 10204 3.1), dimensional report and any third-party inspection.
- Quantities and timing: prototype, first batch, annual volume and delivery schedule.
- Market rules: any lead limit, drinking-water approval, RoHS or REACH requirement in the destination market.
With these details, the grade can be confirmed against the options covered on this page, or an equivalent suggested where it gives better value or performance for the same job.
Frequently asked questions
What is SAE 660 bronze?
SAE 660 is C93200, an 83-7-7-3 leaded tin bronze and the most widely used general-purpose bearing bronze in North America.
What is the difference between SAE 660 and SAE 64?
SAE 64 (C93700, 80-10-10) has more tin and lead than SAE 660, giving higher strength and fatigue resistance together with good anti-seizure properties. It is chosen for heavier loads and higher speeds.
What is LB2 equivalent to?
LB2 corresponds to CC495K (CuSn10Pb10-C) in EN 1982 and C93700 in ASTM.
Why is lead added to bearing bronze?
Lead acts as a built-in solid lubricant, helping the bearing survive moments of poor lubrication, embed dirt and conform to the shaft.
Are bronze bushings cast or machined from bar?
Most standard bushings are machined from continuous-cast or centrifugal-cast tube and bar. Flanged, split or shaped bearings are often sand cast and then machined.
Can leaded bronze bushings run without oil?
They tolerate short periods of poor lubrication better than most metals, but they are not self-lubricating. For dry running, consider graphite-plugged or sintered bearings.
Which bearing bronze is best for dirty environments?
Higher-lead grades such as C93800 (SAE 67, LB1) embed dirt and resist seizure well, provided loads are moderate.
What do you need to quote bronze bushings?
Drawing or dimensions (OD, ID, length, flanges, grooves), grade, quantity, tolerances, whether the bore is finished before or after fitting, and the certificate type.
Other bronze categories
Send your drawing, get a quotation.
DWG, PDF, STEP or a sample photo — with quantity and destination port.